Table 3. LDPE variable response after 150 days P. ostreatus treatment.
Experimental assay | LDPE condition | Young´s Modulus (Mpa) | Yield Strength (MPa) | Roughness (nm) | Weight (mg) | SCA (°) |
---|---|---|---|---|---|---|
Plackett-Burman | T2: LDPE + plasma + P. ostreatus | 59 ± 9 | 8 ± 1 | 4 ± 1 | 4.7 ± 0.5 | 29 ± 7 |
Biodeterioration curve | PBBT150: LDPE + plasma + P. ostreatus | 48 ± 4 | 8 ± 1 | 7 ± 2 | 4.5 ± 0.4 | 17 ± 4 |
PT3: LDPE + plasma | 54 ± 5 | 8 ± 1 | 10 ± 3 | 4.4 ± 0.5 | 21 ± 3 | |
C2:LDPE prístino | 34 ± 6 | 10 ± 2 | 5 ± 1 | 4.4 ± 1.0 | 89 ± 1 |