Skip to main content
. 2018 Sep 12;8(9):718. doi: 10.3390/nano8090718

Table 4.

Initial and secondary sorptivity of cement paste mixes for dry and wet-mix design *.

Samples Initial Sorptivity (mm/s1/2) Reduction Compared to CP (%) Secondary Sorptivity (mm/s1/2) Difference with CP (%)
CP 0.0183 - 0.0035 -
GPD 0.01 0.0147 −19.7 0.0028 −20.0
GPD 0.05 0.0130 −29.0 0.0018 −48.6
GPD 0.1 0.0140 −23.5 0.0027 −22.9
GPD 0.5 0.0170 −7.1 0.0040 +14.3
GPD 1.0 0.0183 0 0.0042 +20.0
GPW0.01 0.0118 −35.5 0.0030 −14.3
GPW0.05 0.0054 −70.5 0.0015 −57.1
GPW 0.1 0.0048 −73.8 0.0012 −65.7
GPW 0.5 0.0126 −31.1 0.0033 −5.7
GPW 1.0 0.0146 −20.2 0.0034 −2.9

* (−ve means reduction, and +ve means increase compared to CP).