Characteristics of prepared P(ESu-co-PAd) copolymers.

Polymer PESu/PPAd Feed 1H-NMR [η] (dL/g) Tm (oC) -COOH (eq/106g)
PESu 100/0 100/0 0.28 120 65
P(ESu-co-PAd) 90/10 90/10 88.9/11.1 0.46 82 54
P(ESu-co-PAd) 80/20 80/20 77.4/22.6 0.50 60 61
P(ESu-co-PAd) 70/30 70/30 67.2/32.8 0.43 35 59
P(ESu-co-PAd) 60/40 60/40 55.6/44.5 0.39 -* 51
P(ESu-co-PAd) 50/50 50/50 46.7/53.3 0.48 -* 58
P(ESu-co-PAd) 40/60 40/60 34.4/65.6 0.50 -* 67
P(ESu-co-PAd) 30/70 30/70 27.3/72.7 0.52 -* 49
P(ESu-co-PAd) 20/80 20/80 18.7/81.3 0.53 -* 43
P(ESu-co-PAd) 10/90 10/90 9.1/90.9 0.62 -* 37
PPAd 0/100 0/100 0.58 43 40

*amorphous material.