Published in final edited form as: Biomaterials. 2018 Jun 18;178:281–292. doi: 10.1016/j.biomaterials.2018.06.023

Table 1.

Composition, fiber diameter, thermal and mechanical properties of electrospun nanofibers.

Fiber code Biomolecules Fiber diameter (nm) Tma (ºC) ΔHma (J/g) Xcb (%) σTSc(MPa) Еd (MPa) εbd (%)
P N.A. 523 ± 129 34 36.1 28.8 7.4 ± 1.1 6.8 ± 1.5 138 ± 18
PC collagen I from calf skin 444 ± 67 35 27.5 24.3 5.8 ± 0.9 4.3 ± 0.7 184 ± 24
a

Tm (melting temperature) and ΔHm (enthalpy change) determinated by the first heating run of DSC curves.

b

Crystallinity (Xc) determinated by the equation: X%=ΔHm/ΔHm0×100% where ΔHm0 is 139.5 J/g for 100% crystalline PCL.

c

σTS = Tensile strength, εb = elongation and Е = Young’s modulus determined by tensile test. Each experiment was done independently for 4 times.