Effects of shear and ultrasonic times on the size, size distribution, and LC loading capacity of LC/PLA nanoparticles a.

Entry Shear Time (min) Ultrasonic Time (min) Mean Diameter (nm) PDI LC Loading Capacity (%)
1 5 10 270.33 ± 5.13 0.17 ± 0.02 45.08
2 10 10 196.93 ± 2.66 0.16 ± 0.015 46.6
3 10 15 190.52 ± 3.74 0.10 ± 0.019 49.4
4 15 10 205 ± 1.39 0.11 ± 0.023 48.21

a PVA concentration was 2%, water–oil ratio was 4:3, PLA concentration was 133 g/L, and LC-PLA ratio was 1:1.