Skip to main content
. 2018 Dec 21;9:3069–3078. doi: 10.3762/bjnano.9.285

Table 5.

EIS data obtained from measurements at a light intensity of 22 mW cm−2 of n-type DSCs containing FTO/TiO2 working electrodes, dye 1 and either electrolytes E2b, E2e or E2c (see Table 3 for compositions). Experimental values of JSC, VOC and η from Table 4 are included for convenience.

Electrolyte Rrec [Ω] Cμ [μF] Rtr [Ω] Inline graphic [ms] Inline graphic [ms] Ld [μm] Rs [Ω] RPt [Ω] CPt [μF] JSC [mA cm−2] VOC [mV] η [%]

E2b
(no MBI)
254.6 233.1 30.0 59.3 6.9 34.9 8.9 9.3 7.4 2.31 339 0.51
E2e
(0.01 M MBI)
138.3 321.9 25.8 44.5 8.3 27.8 9.4 5.7 8.6 2.61 315 0.51
E2c
(0.1 M MBI)
1830 306.7 25.3 561.3 7.8 102.1 9.5 7.7 8.1 0.69 395 0.18