Skip to main content
. Author manuscript; available in PMC: 2019 May 1.
Published in final edited form as: Acta Biomater. 2018 Mar 17;72:35–44. doi: 10.1016/j.actbio.2018.03.008

Table 3.

Mechanical properties of different gelatin-TA crosslinked by silver nitrate (SN) in dry and fully hydrated (swollen) states.

Sample Tensile strength (MPa) Elongation at break (%) Modulus (MPa)

Dry Swollen Dry Swollen Dry Swollen
F-75 33±8 3±0.5a 1.1±0.1 391±19a 3000±540 76±13a
F-75 0.50±0.0b 713±54b 0.12±0.0b
F-100 30±3 - 2.3±1.0 - 1600±500 -
F5-S75 20±6 3.2±0.7a 1.5±0.1 280±49a 1400±360 102±44a
B-75 59±7 3.3±0.7a 1.0±0.1 185±34a 3700±730 48±10a
B-75 0.7±0.1b 348±39b 0.5±0.1b
B5-S75 6.6±0.8a - 111±11a - 173±14a
a

Film samples with water content around 10 wt% (for F2-S75 (F-75), 9.9 wt%, for F5-S75, 11.66 wt%, for B2-S75 (B-75), 12.0 wt%, for B5-S75, 11.55 wt%);

b

Film samples with water content around 50 wt% (for F-75, 51 wt%, for B-75, 45 wt%).