Skip to main content
. 2019 Jan 6;12(1):156. doi: 10.3390/ma12010156

Table 3.

Rounded values for relative decrease/increase [%] for sound (S), aged (A) and consolidated (C) samples and absolute average values of Young’s modulus [kN/mm2], splitting tensile strength [N/mm2], and flexural strength under concentrated load [N/mm2] for St. Margarethen Limestone and Schlaitdorf Sandstone. The graphical visualisation of the same values can be found in Figure 6. All tests were performed six months after consolidation.

Consolidant (S) Sound
± Std.N
(A) Aged
± Std.N
(C) Consolidated
± Std.N
Decrease
(S-A, %)
Increase
(A-C, %)
Magnitude
(S-C, %)
St. Margarethen Limestone Young’s Modulus (kN/mm2) KSE 300 22.7 ± 2.4 9.2 ± 0.7 18.1 ± 1.1 −60 +97 −21
NC-25C 10.0 ± 2.9 22.2 ± 4.1 −56 +123 −2
NC-27CP 13.6 ± 7.9 32.7 ± 9.5 −40 +141 +44
Splitting Tensile Strength (N/mm2) KSE 300 3.3 ± 0.4 1.2 ± 0.2 1.7 ± 0.4 −63 +42 −48
NC-25C 2.1 ± 0.6 +76 −35
NC-27CP 2.5 ± 0.5 +111 −23
Flexural Strength (N/mm2) KSE 300 7.2 ± 1.8 3.8 ± 1.7 5.0 ± 1.8 −47 +31 −31
NC-25C 6.2 ± 1.1 +64 −13
NC-27CP 6.9 ± 1.1 +82 −4
Schlaitdorf Sandstone Young’s Modulus (kN/mm2) KSE 300 15.7 ± 1.9 5.5 ± 1.3 11.7 ± 1.4 −65 +114 −26
NC-25C 6.4 ± 1.0 33.6 ± 3.3 −60 +429 +114
NC-27CP 5.9 ± 0.6 26.8 ± 1.1 −63 +356 +70
Splitting Tensile Strength (N/mm2) KSE 300 3.2 ± 0.2 2.2 ± 0.5 2.5 ± 0.8 −34 +16 −24
NC-25C 4.1 ± 0.5 +89 +25
NC-27CP 3.9 ± 0.4 +80 +19
Flexural Strength (N/mm2) KSE 300 6.6 ± 1.2 2.8 ± 0.6 7.2 ± 1.9 −58 +156 +8
NC-25C 9.0 ± 1.2 +223 +37
NC-27CP 8.4 ± 1.3 +198 +26