Skip to main content
. 2019 Jan 6;12(1):156. doi: 10.3390/ma12010156

Table 4.

Values of water absorption coefficient after one-hour (WAC) [kg·m−2·h−0.5] and ratio of water vapour permeability values (WVP c/a) [kg·m−1·s−1·Pa−1], for sound (s), aged (a) and consolidated (c) specimens of St. Margarethen Limestone (SM) and Schlaitdorf Sandstone (S) evaluated six weeks (6w) and six months (6 m) after treatment.

Stone Treatment WAC(s) WAC(a) WAC(c) (6 w) WAC(c) (6 m) WVPc/a (6 w)
SM KSE 300 4.49 ± 0.05 5.23 ± 0.02 4.52 ± 0.06 4.56 ± 0.03 0.89 ± 0.06
NC-25C 4.50 ± 0.18 5.05 ± 0.11 0.76 ± 0.27 2.99 ± 0.28 0.84 ± 0.03
NC-27CP 4.51 ± 0.15 5.17 ± 0.18 0.47 ± 0.51 0.54 ± 0.26 0.55 ± 0.02
S KSE 300 3.29 ± 0.30 3.66 ± 0.28 0.18 ± 0.15 2.14 ± 0.50 1.75 ± 0.45
NC-25C 2.74 ± 0.72 3.57 ± 0.25 1.65 ± 0.15 1.21 ± 0.28 0.81 ± 0.03
NC-27CP 2.74 ± 0.59 3.53 ± 0.16 0.08 ± 0.04 0.20 ± 0.04 0.35 ± 0.00