Skip to main content
. 2018 Dec 20;10(3):947. doi: 10.1039/c8sc90241k

Table 1. Summary of targeted copolymer compositions, BzMA conversions (% BzMA) as judged by 1H NMR spectroscopy, GPC and DLS data (particle diameter and polydispersity index, PDI) obtained for a series of PBeMA37–PBzMAx diblock copolymers prepared by RAFT dispersion polymerization of BzMA in mineral oil. Synthesis conditions: 90 °C, [PBeMA37 macro-CTA]/[T21s] molar ratio = 5.0, 20% w/w solids. Relevant data for the PBeMA37 macro-CTA are also shown for reference.

Target composition % BzMA THF GPC (vs. PMMA)
DLS at 50 °C
M n/g mol–1 M w/Mn Particle diameter/nm Polydispersity index
PBeMA37 12 400 1.18
PBeMA37–PBzMA50 >99 16 200 1.15 21 0.08
PBeMA37–PBzMA100 >99 22 700 1.15 32 0.01
PBeMA37–PBzMA150 >99 28 100 1.18 37 0.02
PBeMA37–PBzMA200 >99 33 800 1.24 55 0.01
PBeMA37–PBzMA300 >99 43 900 1.38 67 0.01