Table 1.
Material | Details | Deposition/Transfer Techniques | Sheet Resistance (Ω∙sq−1) | Transmission (%) | Ref. |
---|---|---|---|---|---|
CVD graphene | HNO3 doping | Dry transfer/thermal release tape | ~30 (4-layers) | 90 | [12] |
Cu catayst | Polymer-free transfer | 810 (1-layer) 230 (4-layers) |
97.4 (1-layer) 89.4 (4-layers) |
[33] | |
Cu catalyst, HNO3 doping | Clean-lifting transfer | 50 (4-layers) | ~90 (4-layers) | [34] | |
Cu catalyst | Roll-to-Roll green transfer | 97.5 | 5.2k | [35] | |
Ni catalyst | Wet transfer | 500 | 75 | [28] | |
No catalyst | Direct CVD | 370–510 | 82 | [36] | |
No catalyst, 400–600 °C | Direct CVD | 5.2k | 84.6 | [37] | |
Ni/C films on dielectrics | Transfer-free growth | 50 | 96 | [38] | |
Cu-Ni alloy | Wet transfer | 409 | 96.7 | [39] | |
Layer-by-layer, acid-doping | Wet transfer | 80 (4-layers) | 90 (4-layers) | [40] | |
Dual n-doping (NH2-SAMs/DETA) |
Wet transfer | 86 ± 39 | 96 | [41] | |
rGO | Theraml reduction of GO | Spin -coating | 102–103 | 80 | [42] |
rGO/POEGMA layer | Dip-coating | 23.8k | 90 | [43] | |
Thermal reduction of GO | Filtration | 43k | 95 | [44] | |
Thermal reduction of GO | Dip-coating | 1.8 ± 0.08k | 70.7 | [45] | |
Graphene/CNT | Graphene growh on SWNT | Wet transfer | 300 | 96.4 | [46] |
Graphene flake/SWNT | Filtration | 100 | 80 | [47] | |
CVD Synthesis | Wet transfer | ~600 | 95.8 | [48] | |
Thermal reduction of rGO on MWNT | Electrostatic adsorption | 151k | 93 | [48] | |
Chemically converted grpahene/SWNT hybrid suspension | Spin-coating | 636 | 92 | [49] | |
Ultralarge GO/SWNT | Langmuir-Blodgett | 180–560 | 77–86 | [50] | |
Graphan/metallic nano-structure | CVD graphene on AgNW | - | 22 | 88 | [51] |
AgNW on GP | - | 33 | 94 | [52] | |
GP on AgNW | - | 64 ± 6.1 | 93.6 | [53] | |
Roll-to-roll encapsulation | - | 8 | 94 | [54] | |
Graphene/CuNW -Core/shell structure | - | 36 | 79 | [55] | |
Graphene/CuNW Embedded structure |
- | 25 | 82 | [56] | |
Ag-mesh/Graphene | - | 5.39 (GP on mesh) 4.54 (Mesh on GP) |
88.1 (GP on mesh) 89.3 (Mesh on GP) |
[57] | |
Graphene/organics | Graphene/PEDOT:PSS, hybrid ink | Spray coating | 600 | 80 | [58] |
rGO/PEDOT:PSS, hybrid ink | Filtration | 2.3k | 80 | [59] | |
PEDOT:PSS supproting layer on CVD graphene | Wet transfer | 80 ± 4 | 84.6 | [60] | |
Graphene/inorganics | CVD graphene on ITO film | - | 76.46 | 88.25 | [61] |
ITO nanoparticle on CVD graphene | - | 522.21 | 85 | [62] |