Skip to main content
. 2018 Dec 22;9(1):11. doi: 10.3390/nano9010011

Table 4.

Sedimentation, size and polydispersity index of selected SAS in H2O and F-12K medium.

Particle Fluid USD [J/mL] Concentration [μg/mL] Vsed [μm/s] Vsed [mm/d] Xcum [nm] PDI -
P-1 H2O 18 485 0.584 50.49 720 0.55
H2O 270 485 0.041 3.52 318 0.25
F-12K 18 485 0.11 9.51 768 0.45
F-12K 270 485 0.033 2.83 316 0.33
P-2 H2O 18 625 1.083 93.59 695 0.64
H2O 270 625 0.68 58.73 487 0.43
F-12K 18 625 1.041 89.96 656 0.74
F-12K 270 625 0.535 46.19 473 0.43
F-1 H2O 18 985 0.0464 4.01 364 0.16
H2O 270 985 0.0228 1.97 257 0.09
F-12K 18 985 0.0495 4.27 410 0.16
F-12K 270 985 0.0255 2.2 260 0.13
F-2 H2O 18 755 0.0071 0.62 234 0.10
H2O 270 755 0.0033 0.28 177 0.12
F-12K 18 755 0.0071 0.61 235 0.16
F-12K 270 755 0.004 0.34 171 0.10
G-1 H2O 18 800 1.42 123.09 1512 0.89
H2O 270 800 1.35 116.33 1032 0.65
F-12K 18 800 1.03 88.8 2244 0.92
F-12K 270 800 1.21 104.27 1004 0.76
G-2 H2O 18 945 0.35 29.84 805 0.48
H2O 270 945 0.33 28.78 391 0.35
F-12K 18 945 0.3 25.97 652 0.45
F-12K 270 945 0.31 26.96 500 0.35
C-1 H2O n.m. 5000 0.00024 0.021 n.m. n.m.
F-12K n.m. 5000 0.00026 0.023 n.m. n.m.

Particles were dispersed with two ultrasonic dispersion (USD) energies as described in the Method section and measured in either H2O or F-12K medium (Column “Fluid”) at concentrations suitable for DLS measurement (Column: “Concentration”); n.m.: not measured; vsed: sedimentation velocity, xcum: mean particle size, PDI: polydispersity index.