Skip to main content
. 2019 Jan 16;9(1):100. doi: 10.3390/nano9010100

Table 1.

Elemental (CHNS) analysis, ash content, total iron content, and volumetric magnetic susceptibility (κ) of the initial samples (lignite and char) and the samples after high-energy ball milling (magnetic lignite and magnetic char).

Sample Ad (%) Cd (%) Hd (%) Nd (%) Sd (%) Od (%) FeTotal (%) κ (SI Units)
Lignite 13.8 51.9 5.4 0.8 2.3 25.8 - 89 × 10−6
Char 21.6 62.9 3.1 1.0 2.4 9.0 - 223 × 10−6
Magnetic lignite - 46.7 5.4 0.7 2.0 - 7.7 343,333 × 10−6
Magnetic char - 55.5 3.5 0.9 2.2 - 8.5 316,897 × 10−6

Abbreviations: A, ash; d, dry-weight basis; Od, by difference calculated as 100 − (Ad + Cd + Hd + Nd + Sd).