Skip to main content
. 2019 Jan 26;12(3):384. doi: 10.3390/ma12030384

Table 1.

Composition of wood pulp samples. Dosages of surfactants: PVA 3 g/L; SDS 1 g/L; and Tween 6.5 g/L. Total number of trial points is 57. One 21 cm × 35 cm plate-like sample was prepared for each of them from which five parallel test pieces were cut.

Fiber Material Suspension PVA SDS Tween
Pulp Type Consistency [%] Density [kg/m3] Density [kg/m3] Density [kg/m3]
BSKP0 1.00 40.9 47.3 43.2
2.00 48.3 42.6 43.2
2.84 38.3, 80.4 36.6, 37.5, 39.2, 72.2 45.2, 46, 47.5, 95.1
3.00 49, 67.8 48.5, 66.5 48.4, 63.6
4.00 75.5 60.5 69.5
BSKP1 2.13 42.7 42.4 47.3
BSKP2 2.36 39.9 47.6 45.5
CTMP 1.00 46.7 42.9 46.8
2.00 33.7, 43.2, 88.1 39, 42.8, 47.6, 43.6, 71.9 42.6, 47.5, 49.6, 51.3, 96.7
3.00 50.6, 68.3 44.5, 62.3 46.2, 60.6
4.00 74.3 38.3, 56.9 68.5