. 2019 Jan 12;11(1):125. doi: 10.3390/polym11010125

Table 6.

TG data of ceramifiable EVA composites under nitrogen and air atmosphere.

Samples T5% /°C Tmax1/°C Tmax2/°C Residue at 800 °C/%
Nitrogen
EVA0 335 350 468 0.3
EVA1 330 345 470 55.9
EVA2 294 325 460 54.1
EVA3 298 312 460 56.1
EVA4 316 315 460 56.7
EVA5 316 325 460 58.1
EVA6 318 330 460 55.9
EVA7 327 335 460 56.6
Calculate 320 345 468 48.2
Air
EVA0 317 350 460 0.1
EVA1 336 345 475 55.2
EVA2 293 325 456 52.9
EVA3 302 340 470 55.6
EVA4 304 335 471 54.9
EVA5 306 345 464 56.0
EVA6 321 345 471 55.6
EVA7 329 350 472 55.6
Calculate 295 344 460 49.2

T5%: the initial decomposition temperature corresponding to 5% mass loss; Tmax: the temperature at the maximum mass loss rate.