Properties of the poly(ε-caprolactone)-based solutions, diameter of the electrospun fibers and thickness of the annealed films.

Formulation Viscosity
(cP)
Conductivity
(µS/cm)
Surface Tension
(mN/m)
Fiber Diameter
(µm)
Film Thickness
(mm)
PCL 1908.1 ± 41.2 a 0.02 ± 0.00 a 27.2 ± 0.2 a 4.95 ± 0.29 0.09 ± 0.01 a
PCL-SE5 1695.6 ± 36.6 b 0.02 ± 0.00 a 27.4 ± 0.1 a 3.80 ± 0.28 0.10 ± 0.01 a
PCL-SE10 1579.2 ± 33.7 b,c 0.10 ± 0.00 b 27.5 ± 0.1 a 3.65 ± 0.21 0.08 ± 0.01 b
PCL-SE20 1565.9 ± 35.6 c 0.09 ± 0.00 b 24.7 ± 0.1 b 3.31 ± 0.21 0.08 ± 0.01 b

Data are expressed as mean ± standard deviation. Different letters within the same column indicate significant differences among samples (p < 0.05).