Sample %T
800 nm 700 nm 600 nm 500 nm 400 nm 350 nm 300 nm 280 nm 200 nm
P-40-25 79.65 77.57 74.21 66.73 41.49 18.40 0.67 0.10 0.00
0.5%-MMT 74.10 71.22 67.10 59.56 37.83 18.21 0.62 0.04 0.00
1%-MMT 68.55 65.65 61.95 54.25 32.92 18.05 0.53 0.00 0.00
3%-MMT 67.60 63.20 59.40 51.20 27.30 16.40 0.38 0.00 0.00
5%-MMT 62.30 60.00 56.19 47.80 25.10 14.50 0.20 0.00 0.00
0.5%-TiO2 56.15 51.81 45.91 37.64 21.95 11.46 0.10 0.00 0.00
1%-TiO2 41.00 35.30 27.80 20.50 9.20 3.80 0.10 0.00 0.00
3%-TiO2 6.00 3.70 2.10 1.30 0.50 0.00 0.00 0.00 0.00
5%-TiO2 2.00 1.40 1.10 0.80 0.30 0.00 0.00 0.00 0.00