Table 3.

Thermal degradation properties of PLA/PHB/PCL blends with different compositions (wt % PLA/wt % PHB/wt % PCL) obtained by TGA characterization.

PLA/PHB/PCL (wt %) T5 (°C) Tmax (°C) Residual Weight (%)
PHB PLA PCL
100/0/0 328.5 ± 2.6 - 368.5 ± 0.9 - 0.36 ± 0.12
60/40/0 281.8 ± 2.9 291.5 ± 1.2 363.2 ± 0.7 390.6 ± 1.2 4.49 ± 0.24
60/30/10 284.8 ± 3.3 292.5 ± 0.9 363.8 ± 0.8 403.2 ± 1.6 4.23 ± 0.23
60/20/20 285.5 ± 3.4 291.8 ± 1.1 363.6 ± 0.8 408.1 ± 1.3 2.73 ± 0.41
60/10/30 294.3 ± 3.1 297.4 ± 0.6 360.6 ± 1.1 407.4 ± 0.9 1.82 ± 0.54
60/0/40 336.0 ± 2.4 - 366.3 ± 0.6 413.3 ± 0.7 2.54 ± 0.35