Sample ID Lewis AcidXX [Y(OTf)3]0 Tacticity/% Mn/104 Mw/Mn Particle Diameter/nm
Conc./M (mol L−1) m r In 25 °C
P_noLA - 49 51 11.2 1.48 155.3 ± 7.9
I_8 noLA - 48 52 4.01 1.91 216.2 ± 8.7
I_12 noLA - 48 52 3.77 1.99 268.4 ± 44.3
P Y 6 × 10−3 53 47 9.16 1.33 71.0 ± 1.8
I_8 Y 6 × 10−3 52 48 3.11 1.86 332.2 ± 19.6
I_12 Y 6 × 10−3 53 47 3.05 1.87 402.3 ± 28.1