Glass transition temperatures of neat epoxy system and composites with 0.5, 2, and 5 wt % of GO and rGO cured at a temperature of 90 °C.

Sample Peak 1 (°C) Peak 2 (°C) Tg
DGEBA-DDM 110.8 154.9
DGEBA-DDM + 0.5 wt % GO 112.7 170.2
DGEBA-DDM + 2 wt % GO 105.4 176.3
DGEBA-DDM + 5 wt % GO 112.0 176.3
DGEBA-DDM + 0.5 wt % rGO 105.2 162.4
DGEBA-DDM + 2 wt % rGO 107.8 162.4