Skip to main content
. 2017 Nov 12;9(11):603. doi: 10.3390/polym9110603

Table 8.

Service lives (years), required for the tensile strength retention to reach 50%, of both epoxy- and PU-based CFRPs in various conditions in the four cities.

CFRP plates Media Strain level (%) Shanghai 17.0 °C Tianjin 13.7 °C Vancouver 10.3 °C Homer 3.5 °C
Epoxy-based CFRPs Water 0 46.3 57.7 72.9 118.4
30% 20.0 24.2 29.7 45.2
58% 7.0 8.1 9.3 12.6
Seawater 0 32.6 40.2 50.0 78.8
30% 17.2 20.8 25.3 38.2
58% 5.6 6.4 7.3 9.7
PU-based CFRPs Water 58% 13.3 15.4 17.8 24.4
Seawater 58% 9.1 10.3 11.7 15.3