Skip to main content
. 2019 Feb 21;11(2):380. doi: 10.3390/polym11020380

Table 3.

Cone calorimetric data for EP and EP/polysulfone composites at 50 kW·m−2.

Sample TTI
(s)
PHRR
(kW·m−2)
THR
(MJ·m−2)
TML
(%)
TSR
(m2)
THR/TML
(MJ·m−2·g−1)
TSR/TML
(g−1)
TCOR/TML
(g·g−1)
EP 50 1712 83.7 93.0 22.4 3.85 117 0.11
EP/ArPN2 29 847 61.5 80.2 18.3 3.27 110 0.15
EP/ArPO2 32 608 42.7 82.7 19.2 2.31 117 0.18
EP/ArOPN2 30 546 59.4 77.1 11.4 3.42 75 0.14
EP/ArOPO2 30 726 55.3 80.8 14.8 3.09 94 0.14