Combustion data of untreated and QL-treated PET-COT by cone calorimetry at different heat fluxes [29].

Sample TTI ± σ [s] PHRR ± σ [kW/kg] ΔPHRR [%]
Heat flux = 25 kW/m2
PET-COT (340 g/m2) 49 ± 8 427 ± 20 -
1 QL 68 ± 9 305 ± 23 −29
5 QL 57 ± 6 307 ± 4 −28
10 QL 65 ± 10 270 ± 13 −37
Heat flux = 35 kW/m2
PET-COT 26 ± 5 482 ± 23 -
1 QL 18 ± 2 303 ± 5 −37
5 QL 24 ± 4 287 ± 12 −40
10 QL 36 ± 14 275 ± 64 −43
Heat flux = 50 kW/m2
PET-COT 14 ± 2 638 ± 41 -
1 QL 12 ± 1 544 ± 24 −15
5 QL 14 ± 1 476 ± 10 −25
10 QL 14 ± 2 435 ± 26 −32