Combustion data of untreated and BL-treated PET-COT by cone calorimetry (35 kW/m2) [30].

Sample TTI ± σ [s] PHRR ± σ [kW/m2] ΔPHRR [%]
PET-COT (340 g/m2) 22 ± 2 170 ± 3 -
5 BL Chi/APP 12 ± 3 162 ± 6 −5
10 BL Chi/APP 17 ± 6 138 ± 16 −19
20 BL Chi/APP 17 ± 4 128 ± 3 −25
5 BL Silica/APP 33 ± 12 178 ± 10 5
10 BL Silica/APP 31 ± 5 168 ± 8 −1
20 BL Silica/APP 31 ± 9 172 ± 9 +1