Results of DSC scans at 10 °C/min, for the neat epoxy resin and epoxy resins with 3 wt % of different carbon nanofillers: enthalpy changes, normalized with respect to the resin weight (∆HU), peak temperature (Tpeak), and fraction of catalyzed reaction.

Sample HU (J/g) Tpeak °C Amine catalyzed fraction (%)
Epoxy 313.9 ± 1.1 113.7 ± 0.9 0
Epoxy + oCB-1 (O/C = 0.16) 327.5 ± 2.2 96.5 ± 0.8 12
Epoxy + oCB-2 (O/C = 0.83) 383.8 ± 1.1 96.2 ± 0.7 34
Epoxy + oCB-3 (O/C = 0.91) 352.5 ± 1.7 88.7 ± 1.1 56
Epoxy + eGO (O/C = 0.62) 374.4 ± 2.3 95.0 ± 0.7 29