Temperature and height of the loss modulus (Tβ) and (Tα) peaks of neat and nanofilled PP fibers as a function of the fumed silica volume fraction. Effective volume fraction of dispersed phase, (фe) and B parameter were calculated according to the model proposed by Sumita et al. [63].

Material Tβ/(°C) E″ Peak (MPa) Tα/E″ Peak (°C)/(MPa) фe B
DR = 10 DR = 15 DR = 10 DR = 15 DR = 10 DR = 15 DR = 10 DR = 15
PP −28/1646 −25/1408 67/706 69/1378 - - - -
AR974-0.25 −27/1556 −24/1568 65/1368 71/1492 0.482 0.087 193.0 34.9
AR974-0.5 −27/1874 −22/1603 64/1164 69/1650 0.392 0.175 78.4 35.1
AR974-1 −20/1618 −25/2115 73/748 70/1841 0.053 0.253 5.3 25.3
AR974-2 −19/1528 −22/1689 74/410 76/1331 −0.70 −0.013 −35.1 −0.6