Roughness of the different dental implants.

Ti Alloys Before Shot Blasting After Shot Blasting
Ra (µm) Pc (cm−1) Ra (µm) Pc (cm−1)
Ti-6Al-4V 0.56 ± 0.14 8.2 ± 0.3 1.99 ± 0.41 98.3 ± 2.4
Ti cp 0.43 ± 0.11 9.9 ± 1.2 2.33 ± 0.54 70.9 ± 9.2
Ti-15Zr 0.33 ± 0.07 8.4 ± 1.7 2.23 ± 0.76 88.1 ± 11.1
Ti-19.1Nb-8.8Zr 0.44 ± 0.10 7.3 ± 1.6 1.74 ± 0.25 82.1 ± 10.0
Ti-41.2Nb-6.1Zr 0.33 ± 0.07 8.8 ± 1.2 1.83 ± 0.33 92.1 ± 13.0
Ti-25Hf-25Ta 0.23 ± 0.05 6.9 ± 2.2 2.33 ± 0.53 70.9 ± 9.2