Electrospun PLA-PHB fibers and their composites.

Formulations PLA
(wt%)
PHB
(wt%)
OLA
(wt%)
Cat
(wt%)
Fibers Diameter (nm) Dinamic Viscosity (η)
(Pa.s)
PLA-PHB 75 25 - - 215 ± 67 0.12 ± 0.01
PLA-PHB-OLA 63.75 21.25 15 - 260 ± 78 0.06 ± 0.01
PLA-PHB-Cat1 74.25 24.75 - 1 405 ± 143 0.13 ± 0.03
PLA-PHB-OLA-Cat1 63.0 21.0 15 1 228 ± 57 0.06 ± 0.02
PLA-PHB-Cat3 72.75 24.25 - 3 400 ± 116 0.14 ± 0.01
PLA-PHB-OLA-Cat3 61.5 20.5 15 3 206 ± 57 0.07 ± 0.01