Samples | Maximum Tensile Stress (MPa) | Young's Modulus (MPA) |
Elongation at Break (%) |
---|---|---|---|
PLA | 1.15 | 3.8 | 18.50 |
PLA/2.5 wt% EnHA | 3.65 | 39.4 | 9.50 |
PLA/5 wt% EnHA | 5.40 | 72.2 | 7.70 |
PLA/10 wt% EnHA | 2.3 | 39.3 | 5.00 |
Samples | Maximum Tensile Stress (MPa) | Young's Modulus (MPA) |
Elongation at Break (%) |
---|---|---|---|
PLA | 1.15 | 3.8 | 18.50 |
PLA/2.5 wt% EnHA | 3.65 | 39.4 | 9.50 |
PLA/5 wt% EnHA | 5.40 | 72.2 | 7.70 |
PLA/10 wt% EnHA | 2.3 | 39.3 | 5.00 |