Details of chemicals and experimental conditions for the preparation of nanocomposite structures (Co@AgNPs).

sample precursor reducing agent stabilizing agent reaction conditions
S0 cobalt acetate (48 mM, 25 ml) hydrazine hydrate (0.4 ml), ethylene glycol (25 ml), added dropwise PVP (0.25 mM, 50 ml) heated up to 195°C under refluxing conditions with constant stirring (100 r.p.m.)
S1 silver acetate (0.01 g) added to S0 mixed by stirring (100 r.p.m.) at room temperature
S2 silver acetate (0.1 g) added to S0 mixed by stirring (100 r.p.m.) at room temperature
S3 silver acetate (0.2 g) added to S0 mixed by stirring (100 r.p.m.) at room temperature