Split tensile strength of concrete with varying GO nanosheet contents.

Mix ID GO (%) Split Tensile Strength (MPa) Increase at 28 Days (%)
7 Days 14 Days 28 Days
GCO0 0.00 1.98 2.35 2.62 0.00
GCO2 0.02 2.43 2.77 3.04 16.18
GCO3 0.03 2.58 2.98 3.27 24.81
GCO4 0.04 2.45 2.81 3.11 18.75
4CO6 0.06 2.41 2.76 3.04 15.95
GCO8 0.08 2.32 2.72 3.01 14.79