Skip to main content
. 2019 Jun 17;11(6):1052. doi: 10.3390/polym11061052

Table 1.

Thermoelectric properties of PEDOT:PSS/Se and control films at room temperature.

System Electrical Conductivity
(σ) / S cm−1
Seebeck Coefficient
(S) / μV K−1
Power Factor
(S2σ) / μW cm−1K−2
Se a 1.4 x 10−7 ~1000 b ~0.0014
PEDOT:PSS 0.29 (±0.17) 24.9 (±0.9) 1.7
PEDOT:PSS/Se 0.37 (±0.19) 45.5 (±3.5) 9.5
PEDOT:PSS/Se c 0.71 (±0.10) 44.5 (±6.7) 15.0

a The Se pellet was prepared by compression of finely ground Se powders. b Bulk Seebeck coefficient of Se crystals [12,13]. c Thermally annealed films of PEDOT:PSS/Se at 120 °C for 15 min.