Skip to main content
. 2018 Aug 31;3(8):10278–10285. doi: 10.1021/acsomega.8b01461

Table 1. Wetting Properties for Sprayed F-PETMP/SiO2 Thiol–Acrylate Thin Films.

SiO2 (%) (y) WCA (deg) WSA (deg) OCA (deg) OSA (deg)
F-PETMP(20)/SiO2(y)
30 18.7 ± 0.4   135.5 ± 1.6  
40 14.5 ± 0.8   136.9 ± 1.9  
50 0   140.1 ± 2.0  
60 0   135.7 ± 1.1  
F-PETMP(30)/SiO2(y)
30 45.7 ± 1.1   138.7 ± 1.7  
40 32.1 ± 0.5   144.2 ± 2.1  
50 0   155.6 ± 1.0 10 ± 1
60 0   155.3 ± 0.9 12 ± 1
F-PETMP(40)/SiO2(y)
30 103.6 ± 0.7   140.2 ± 0.6  
40 121.9 ± 1.1   150.5 ± 1.5  
50 142.8 ± 0.9   156.1 ± 0.9 7 ± 2
60 146.7 ± 1.3   155.9 ± 0.8 7 ± 1
F-PETMP(50)/SiO2(y)
30 134.3 ± 0.6   148.9 ± 1.4  
40 141.8 ± 1.2   150.5 ± 0.7 12 ± 2
50 150.6 ± 0.8 5 ± 1 158.6 ± 0.8 7 ± 1
60 156.6 ± 0.9 5 ± 1 156.7 ± 1.0 8 ± 1