Skip to main content
. 2019 Jul 22;12(14):2331. doi: 10.3390/ma12142331

Table 4.

List of DMLS parameters and properties of Ti6Al4V alloy heat treated at 850 °C meeting the criteria of ASTM F 1142 standard for implantable biomaterials.

P
[W]
V
[mm/s]
Rm [MPa] Re [MPa] A [%] E [GPa] Es
[J/mm3]
P
[%]
ZX XZ ZX XZ ZX XZ ZX XZ
150 500 1056 ± 13 1052 ± 12 954 ± 10 950 ± 8 13.4 ± 0.5 13.2 ± 0.6 106.5 ± 1.3 106.2 ± 0.6 100 0.46
170 500 1074 ± 13 1069 ±10 974 ± 9 973 ± 7 13.7 ± 0.6 13.6 ± 0.5 107.5 ± 0.7 107.5 ± 0.8 113 0.27
190 500 1080 ± 10 1077 ± 11 982 ± 9 980 ± 9 14.3 ± 06 14.1 ± 0.7 108.0 ± 1.2 108.7 ± 0.5 127 0.16
210 700 1062 ± 12 1055 ± 10 962 ± 9 954 ± 8 13.5 ± 0.5 13.3 ± 0.8 107.2 ± 1.0 107.4 ± 0.9 100 0.45