Skip to main content
. 2019 Aug 6;4(8):13270–13278. doi: 10.1021/acsomega.9b01442

Table 1. Electrospinning Conditions and Fiber Morphology for PVA and the Blend PVA/BSA.

feed solution voltage (kV) feed rate (mL/h) tip-collector distance (cm) note on sample morphology
10 wt % PVA 12–24 0.1–0.4 18–25 highly beaded and defective fibers
12 wt % PVA 15–21 0.05–0.1 20–30 defect-free fibers and very few beaded fibers
14 wt % PVA 15–18 0.05–0.2 25–28 homogeneous and defect-free fibers
15 wt % PVA 15–19 0.1–0.3 12–18 homogeneous and defect-free fibers
16 wt % PVA 15–17 0.2 13–18 few defect-free fibers; low production yield
12 wt % PVA (10–100)% BSA 17–19 0.3 18 homogeneous and defect-free fibers
13 wt % PVA (10–100)% BSA 17–19 0.3 18 homogeneous and defect-free fibers
14 wt % PVA (10–100)% BSA 17–19 0.3 18 homogeneous and defect-free fibers