Table 1. Tensile Properties of SBR and SBR/CNF Nanocomposites.

samples modulus (MPa) failure strength (MPa) failure strain
neat SBR 1.67 ± 0.06 3.20 ± 0.71 7.14 ± 1.31
industrial SBR 7.35 ± 0.30 16.10 ± 0.91 4.08 ± 0.25
3% CNF 2.75 ± 0.25 4.18 ± 0.34 5.04 ± 0.55
7% CNF 10.33 ± 1.73 8.06 ± 0.95 7.86 ± 0.88
9% CNF 12.29 ± 2.23 6.16 ± 0.15 2.39 ± 0.39
3% TC-CNF 4.71 ± 0.34 5.86 ± 0.20 4.08 ± 0.24
7% TC-CNF 13.01 ± 1.40 7.43 ± 0.16 3.23 ± 0.16
9% TC-CNF 12.79 ± 1.58 10.32 ± 0.39 2.76 ± 0.14
3% A4-CNF 3.65 ± 0.49 6.30 ± 0.31 5.91 ± 0.98
7% A4-CNF 12.65 ± 3.17 10.49 ± 0.42 2.17 ± 0.36
9% A4-CNF 22.14 ± 2.78 12.77 ± 0.16 1.57 ± 0.16
3% A4-CNF-Tola 4.63 ± 0.23 7.04 ± 0.61 4.21 ± 0.21
7% A4-CNF-Tola 12.00 ± 2.57 11.16 ± 0.46 2.60 ± 0.15
9% A4-CNF-Tola 26.75 ± 3.36 12.26 ± 0.35 1.79 ± 0.16
7% T3-CNF 9.78 ± 1.95 9.03 ± 0.29 3.57 ± 0.48
7% T11-CNF 11.51 ± 1.76 8.66 ± 0.57 2.04 ± 0.30
7% A10-CNF 9.67 ± 1.18 9.37 ± 0.34 3.32 ± 0.12
a

Nanocomposite samples prepared using toluene as the solvent.