Table 3.

Mechanical properties data including elastic modulus (kPa) and ultimate tensile stress (kPa) with n = 4. Samples are grouped by the ratio of PEGDA to AA and by the overall concentration for statistical comparisons. (* indicates a statistically significant difference with p < 0.05).

Hydrogel Sample Elastic Modulus (kPa) Ultimate Tensile Stress (kPa)
100% PEGDA 96.3 ± 18.7 26.0 ± 5.6*
1:4 PEGDA:AA 78.4 ± 7.3 56.2 ± 4.5
1:8 PEGDA:AA 89.1 ± 8.8 47.0 ± 11.2
1:12 PEGDA:AA 90.0 ± 13.4 61.4 ± 13.7
1:16 PEGDA:AA 77.8 ± 7.0 44.9 ± 9.5
 
0.9 g/mL 67.3 ± 4.3* 22.7 ± 8.7
1.8 g/mL 96.2 ± 6.1* 23.0 ± 3.9
2.7 g/mL 191.8 ± 20.3 36.6 ± 3.4
3.6 g/mL 213.6 ± 7.0 42.9 ± 23.0