Table 2. Thermal Transitions by DSC and DMA of Printed Recycled and COTs PP/Cellulose Composites.
sample | Tc (°C) | Tm (°C) | Tg (tan δ) | % crystallinitya |
---|---|---|---|---|
rPP ctrl | 121.8 | 167.8 | 8.7 | 31.5 |
rPP SSSP ctrl | 117.7 | 164.0 | 13.2 | 25.6 |
rPP 5% WP | 123.6 | 166.7 | 12.2 | 31.5 |
rPP 10% WP | 122.6 | 167.8 | 11.9 | 27.3 |
rPP 20% WP | 120.9 | 162.8 | 11.0 | 20.3 |
rPP 5% CB | 124.4 | 167.2 | 11.7 | 29.2 |
rPP 10% CB | 125.3 | 169.3 | 10.0 | 25.7 |
rPP 20% CB | 126.7 | 164.3 | 10.3 | 19.0 |
rPP 5% WF | 127.4 | 164.8 | 12.4 | 25.8 |
rPP 10% WF | 124.5 | 168.8 | 14.2 | 24.0 |
rPP 20% WF | 125.7 | 163.5 | 13.0 | 19.0 |
cPP ctrl | 111.9 | 163.7 | 14.5 | 39.2 |
cPP SSSP ctrl | 118.4 | 164.4 | 12.3 | 41.3 |
cPP 5% WP | 121.7 | 165.2 | 12.1 | 36.3 |
cPP 10% WP | 119.4 | 166.2 | 8.6 | 31.4 |
cPP 20% WP | 121.2 | 166.1 | 9.0 | 23.8 |
cPP 5% CB | 117.7 | 164.6 | 9.0 | 38.0 |
cPP 10% CB | 118.6 | 167.1 | 11.1 | 37.0 |
cPP 20% CB | 118.6 | 164.8 | 10.6 | 25.0 |
cPP 5% WF | 121.4 | 164.5 | 11.2 | 37.4 |
cPP 10% WF | 117.4 | 168.7 | 10.1 | 38.5 |
cPP 20% WF | 117.7 | 163.6 | 10.2 | 30.4 |
Fractional, WP = waste paper, CB = cardboard, WF = wood flour.