Specimens’ concentration in phr (parts per hundred per resin per weight), activation energy values and fitted parameters for all examined systems.

ZnFe2O4 Nanocomposites IP α-relaxation
EA (eV) TV (K) B
neat epoxy - 315.9 17.5
1 phr - 313.3 19.3
3 phr - 311.6 19.4
5 phr 0.549 311.2 18.6
10 phr 0.649 307.7 18.0
15 phr 0.748 303.0 17.6
20 phr 0.832 306.1 18.0