Thermal properties of PLA–wool FRP studied materials.

Formulation TGA Assessment DSC Assessment
T5 (°C) Tmax (°C) Mass Loss at 300 °C (%) Mass Loss at 350 °C (%) Tg (°C) Tcc (°C) Tm (°C) Xc (%)
PLA–MLO 327.2 ± 0.4a 364.9 ± 2.5a 2.8 ± 0.2a 21.6 ± 0.6a 60.7 ± 0.6a 105.5 ± 1.2a 170.6 ± 0.9a 19.9 ± 0.9a
PLA–MLO–UW 327.0 ± 1.8a 366.4 ± 2.6a 1.9 ± 0.6a,b 23.2 ± 1.9a 58.6 ± 1.0a 105.2 ± 0.5a 168.1 ± 1.2a 19.2 ± 1.3a
PLA–MLO–WA 325.3 ± 1.1a 365.9 ± 3.3a 1.7 ± 0.4b 22.5 ± 0.9a 60.1 ± 1.0a 111.5 ± 2.0b 169.7 ± 0.7a 16.7 ± 0.7b
PLA–MLO–WB 326.8 ± 0.7a 366.9 ± 1.9a 2.6 ± 0.3a,b 21.0 ± 1.2a 60.2 ± 1.0a 111.3 ± 0.5b 170.1 ± 0.5a 16.4 ± 0.8b
PLA–MLO–WC 324.2 ± 1.6a 365.9 ± 0.3a 2.4 ± 0.4a,b 23.1 ± 1.4a 60.4 ± 1.4a 111.6 ± 2.5b 170.3 ± 1.4a 16.1 ± 0.5b
PLA–MLO–WD 324.9 ± 1.2a 356.9 ± 2.6a 1.7 ± 0.2b 32.9 ± 5.7b 60.2 ± 1.0a 110.2 ± 0.6b 169.8 ± 0.6a 17.5 ± 0.6b