Table 1.

Cryo-Polymerizations for the Preparation of P(LA-co-EGDMA) Cryogels at [M]0 = 0.6 mol/L.

Cryogels Code a EGDMA (mol%) b Temperature (°C) Swelling Ratio c Gel Fraction (%)
C-63p4 3 +4 21–22 79
C-65p4 5 +4 14–15 80
C-67p4 7 +4 12–13 81
C-63p2 3 +2 15–16 95
C-65p2 5 +2 12–13 98
C-67p2 7 +2 10–11 97
C-63z0 3 0 not measured 31
C-65z0 5 0 not measured 51
C-67z0 7 0 not measured 54

a: The first and second Arabic number represents [M]0 and molar percent of EGDMA, respectively. The annotation of “p4”, “p2” and “z0” indicates temperatures of +4, +2 and 0 °C, respectively. b: The EGDMA molar percentage (fEGDMA) is based on the total moles of lauryl acrylate (LA) and EGDMA. c: The saturated swelling ratio of cryogels in toluene is presented.