Summary of the steps adopted for methods A, B and C for polishing of the CNF/LDPE samples.

Paper Speed (rpm) Time (minutes) Lubricant
Method A
SiC–P200 180 5 Water
SiC–P400 180 8 Water
SiC–P800 180 8 Water
SiC–P1200 180 10 Water
SiC–P2500 180 10 Water
Method B
SiC–P400 180 5 Water
SiC–P600 180 8 Water
SiC–P1200 180 8 Water
SiC–P2500 180 8 Water
Microcloth 160 8 Diamond suspension 1 μm size
Microcloth 160 8 Alumina suspension 0.05 μm size
Method C
SiC–P400 150 5 Water
SiC–P800 150 8 Water
SiC–P1200 150 8 Water
SiC–P2500 180 8 Water
Microcloth 180 12 Diamond suspension 1 μm size
Microcloth 180 12 Alumina suspension 0.3 μm size
Microcloth 180 12 Alumina suspension 0.05 μm size