Cone calorimeter test results of PBT/PET blend and flame-retardant PBT/PET materials.

Sample PHRR (kW/m2) Mean-EHC (MJ/kg) THR (MJ/m2) Mean-CO2Y(kg/kg) TSR (m2/m2)
TAD0 1087.7 17.1 92.0 1.48 1530.9
TAD4 885.1 8.6 94.2 0.91 1853.5
TAD8 777.9 8.9 91.0 0.92 1944.3
TAD12 616.7 10.4 84.3 0.99 2105.0
TAD16 486.7 10.6 72.1 1.05 2236.5
TAD6EG6 390.4 7.8 84.7 0.67 2622.9
EG12 435.2 10.2 78.3 0.83 2412.5