Table 2.
Sample | α-Al2O3, wt.% | γ-Al2O3, wt.% |
---|---|---|
Al powder | - | - |
Air 750 °C | 20.2 | 2.4 |
Ar 750 °C | - | 4.6 |
Ar 800 °C | - | 3.8 |
Ar 850 °C | 1.5 | 4.3 |
Ar 900 °C (shrink part of the foam) | 28.8 | 7.4 |
Sample | α-Al2O3, wt.% | γ-Al2O3, wt.% |
---|---|---|
Al powder | - | - |
Air 750 °C | 20.2 | 2.4 |
Ar 750 °C | - | 4.6 |
Ar 800 °C | - | 3.8 |
Ar 850 °C | 1.5 | 4.3 |
Ar 900 °C (shrink part of the foam) | 28.8 | 7.4 |