Table 2.
Mean coefficient of thermal expansion α CTE for SLM-fabricated Invar, Invar 36®[2], and stress-relieved SLM-fabricated Invar
| Temp (°C) | 30–100 | 30–150 | 30−200 | 30–260 | 30–279 |
|---|---|---|---|---|---|
| SLM z | −0.355 | 0.164 | 0.889 | 2.77 | 3.56 |
| SLM x–y | −0.471 | 0.098 | 0.767 | 2.58 | 3.34 |
| Invar 36® | 1.6a | 2.0 | – | 4.1 | – |
| SLM stress-relieved z | 1.00 | 1.34 | 1.85 | 2.96 | 3.68 |
| SLM stress-relieved x–y | 0.70 | 0.99 | 1.53 | 2.74 | 3.36 |
aFor temperature range 25–93 °C
Units are (10−6/ °C); uncertainty of measurement is ±0.01 10−6/ °C