Skip to main content
. 2020 Jan 22;10:2986. doi: 10.3389/fmicb.2019.02986

TABLE 1.

Molecular weight and polydispersity index of the PE-PU-A copolymer during cultivation with the BP8 community.

Culture time Mn Mw PDI
(days) (g/mol) (g/mol)
Non-inoculated 101,8968,098 208,4907,600 2.00.3
5 96,798712 210,83726,098 2.20.1
10 89,2585,825 223,58118,736 2.50.3
15 82,5771,168 229,37226,416 2.70.3
20 73,4069,225 187,92550,737 2.40.3
25 65,609990 169,9255,080 2.60.2

Number-average molecular weight (Mn), weight-average molecular weight (Mw) and polydispersity index (PDI) were calculated by Gel permeation chromatography with monodisperse polystyrene calibration standards and using THF as eluent. n = 3.