Table 1.
Parameter | Orthogonal | A05W2 | A0.5W3 | A0.5W4 | A0.75W4 | A1W4 |
---|---|---|---|---|---|---|
Amplitude (mm) | - | 0.5 | 0.5 | 0.5 | 0.75 | 1 |
Wavelength (mm) | - | 2 | 3 | 4 | 4 | 4 |
Strut diameter (μm) | 533 ± 9 | 497 ± 73 | 490 ± 36 | 513 ± 30 | 510 ± 32 | 460 ± 58 |
Strut spacing 1 (μm) | 395 ± 6 | 277 ± 59 | 350 ± 53 | 396 ± 72 | 308 ± 72 | 336 ± 103 |
Struts per layer | 16 | 15 | 15 | 15 | 15 | 15 |
Temperature 2 (°C) | 80 | 80 | 80 | 80 | 80 | 80 |
Print pressure (Pa) | 7 × 105 | 7 × 105 | 7 × 105 | 7 × 105 | 7 × 105 | 7 × 105 |
Print speed (mm/s) | 4 | 4 | 6 | 5 | 5 | 5 |
E 3 (MPa) | 12.4 ± 0.3 | 10.5 ± 0.5 | 11.5 ± 0.2 | 9.5 ± 0.2 | 10.7 ± 0.2 | 11.3 ± 0.5 |
Porosity 4 (%) | 56.3 ± 0.7 | 56.5 ± 1.2 | 55.9 ± 0.3 | 61.7 ± 0.9 | 57.6 ± 0.5 | 57.2 ± 3.1 |
1 Strut-to-strut distance. 2 Print temperature. 3 Young’s modulus from compression tests. 4 Micro-CT results.