Copolyester Mn Mw Tg (°C) Tc (°C) Tm (°C)
1 PBS 7500 21,470 −33 76 114
2 BS91CL9 8790 21,640 −36 61 104
3 BS78CL22 6580 18,000 −40 46 93
4 BS66CL34 7830 19,700 −44 14 73
5 BS62CL38 9750 27,300 −45 12 70
6 BS55CL45 8970 24,700 −46 7 62
7 BS51CL49 7400 23,500 −47 4 58
8 BS45CL55 8000 17,300 −48 −5/−22 13/49
9 BS38CL62 11,000 24,300 −50 −13 17
10 BS34CL66 10,000 29,900 −51 −10 18
11 BS27CL73 11,540 28,700 −53 −8 19
12 BS11CL89 6300 19,500 −56 10 36
13 PCL 5400 17,400 −60 34 55