. 2020 Jan 23;13(3):543. doi: 10.3390/ma13030543

Table 5.

Degradation temperature, weight loss, and residue for different post-consumer rPP composites.

Sample 23–310 °C 310–560 °C 560–700 °C 700 °C Onset Degradation
Wt. Loss
(%)
Wt. Loss
(%)
Tmax.1
(°C)
Tmax.2
(°C)
Wt. Loss
(%)
Tmax.3
(°C)
Wt. Loss
(%)
Ti
(°C)
Wt. Loss
(%)
rPP 1.94 83.35 463.4 - 5.04 633.4 9.68 445.3 96.01
SBS 0.29 99.26 452.3 - 0.23 - 0.22 415.8 99.69
rPP/SBS 1.62 85.14 461.7 - 4.51 641.8 8.72 434.9 96.72
rPP/SBS/GB 5 1.28 84.46 463.7 - 4.46 645.1 9.80 437.0 97.11
rPP/SBS/GB 20 1.16 82.52 464.9 - 4.35 653.1 11.98 437.6 97.31
SIS 0.90 98.63 375.3 423.6 0.03 - 0.44 353.0 96.86
rPP/SIS 1.46 85.40 370.9 458.4 4.47 641.3 8.6 429.5 95.97
rPP/SIS/GB 5 1.35 84.67 374.7 461.5 4.51 649.9 9.47 431.8 96.17
rPP/SIS/GB 20 1.26 82.76 373.3 460.8 4.31 648.2 11.67 431.0 96.30