Skip to main content
. 2020 Mar 3;7:8. doi: 10.1186/s40580-020-0218-x

Table 1.

Carrier concentration, mobility and TE properties of the annealed films at 303 K

Types of films Sb2Te3 Bi2Te3 Bi2Te3/Au multilayer Bi2Te3/Pt multilayer
Type of carrier Holes Electrons Electrons Electrons

Carrier concentration

[cm−3]

(2.9 ± 0.3) × 1020 (1.8 ± 0.2) × 1021 (6.8 ± 0.1) × 1021 (2.0 ± 0.2) × 1021

Carrier mobility

[cm2 V−1 s−1]

5.7 ± 0.2 8.77 ± 0.4 1.5 ± 0.1 13.2 ± 0.2

Seebeck coefficient

[μV K−1]

148.4 ± 1.0 62.0 ± 0.3 55.0 ± 1.1 107.05 ± 1.1

Electrical conductivity

[S cm−1]

252 ± 6 2638 ± 58 1525 ± 81 4054 ± 11

Power factor

[μW cm−1 K−2]

5.5 ± 0.6 10.1 ± 0.4 4.61 ± 0.7 46.5 ± 0.5